Vigil Antislip

Test Results

Resistance to Impact : RESULTS 196kg.cm.

Test Method ASTM D2794
Height Level
Condition
 
kg.cm
1
2
3
4
5
Low
192
Crack
No
No
No
No
Medium
196
No
Crack
No
No
Crack
High
200
No
Crack
No
Crack
Crack

Slip Resistance :

Test Method ASTM D4518
Condition
Result
Dry
0.53
Wet
0.50
Oiled
0.49
Oiled After Impact
0.41

Test Method DIN 51130
Grade
Result
Commercial
R -13
Industrial
R -12
Offshore
R -12

Test Method AS/NZ 3661.1
.
Commercial
Industrial
Offshore
Dry Leather
1.30
1.50
1.80
Dry Rubber
1.30
1.30
1.90
Wet Rubber
0.95
0.85
0.85

Resistance to Delamination : RESULTS 1.9 - 2.3 N/sq.mm. Test Method BS 3900 Pt. E10.

Resistance to Abrasion : Result > 313.6 g/mm. Test Method ASTM D658.

Chemical Resistance of Resins :

Javel Water (NaCl, Sodium hypochlorite) 14%

Sulphuric acid

10%
Nitric acid 30%
Formic acid 10%
Acetic acid 10%
Latic acid 5%
Petrol (tetraethyl lead fuel)  
Toluene  
Styrene  
1.1, 1-trichloroethane  
Skydrol 500A (hydraulic fluid for aircraft)  
Test periods in week  
   
resistant
slightly softened

For more information please contact us.